EN 10028-3 Grade P460N normalized and stress-relieved
Equivalent material: GB 15MnVNR, GB L27153, GB 18MnMoNbR, GB A05189, DIN P460N, ASTM C, UNS K12202, ASTM A612, ASTM A737 Grade C, DIN StE47, DIN 1.8905, DIN StE 460, BS P460N, JIS SM53B, JIS SM53C, JIS SM520B, JIS SM520C, JIS E460DD, EN 1.8905, ISO E460DD, ASTM F70, ASTM Grade LF6 Class 1
EN 10028-3 Grade P460N normalized and stress-relieved general
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 20 °C | Density of 7.84 g/cm³ | normalized and stress-relieved | EN 10028-3 | Sheet |
EN 10028-3 Grade P460N normalized and stress-relieved thermal
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | -100 °C | Coefficient of thermal expansion of 1.05e-05 1/K | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 20 °C | Coefficient of thermal expansion of 1.15e-05 1/K | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 100 °C | Coefficient of thermal expansion of 1.21e-05 1/K | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 200 °C | Coefficient of thermal expansion of 1.27e-05 1/K | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 300 °C | Coefficient of thermal expansion of 1.32e-05 1/K | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 400 °C | Coefficient of thermal expansion of 1.36e-05 1/K | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 500 °C | Coefficient of thermal expansion of 1.4e-05 1/K | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 600 °C | Coefficient of thermal expansion of 1.44e-05 1/K | normalized and stress-relieved | EN 10028-3 | Sheet | - |
Max service temperature | - | Max service temperature of 500 °C | - | - | - | Typical for Carbon Steel |
Melting point | - | Melting point of 1480 - 1526 °C | - | - | - | Typical for Low Carbon Steel |
Specific heat capacity | -100 °C | Specific heat capacity of 423 J/(kg·K) | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 20 °C | Specific heat capacity of 461 J/(kg·K) | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 100 °C | Specific heat capacity of 479 J/(kg·K) | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 200 °C | Specific heat capacity of 499 J/(kg·K) | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 300 °C | Specific heat capacity of 517 J/(kg·K) | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 400 °C | Specific heat capacity of 536 J/(kg·K) | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 500 °C | Specific heat capacity of 558 J/(kg·K) | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 600 °C | Specific heat capacity of 587 J/(kg·K) | normalized and stress-relieved | EN 10028-3 | Sheet | - |
Thermal conductivity | -100 °C | Thermal conductivity of 34.7 W/(m·K) | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 20 °C | Thermal conductivity of 39.7 W/(m·K) | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 100 °C | Thermal conductivity of 40.9 W/(m·K) | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 200 °C | Thermal conductivity of 41 W/(m·K) | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 300 °C | Thermal conductivity of 39.9 W/(m·K) | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 400 °C | Thermal conductivity of 38.2 W/(m·K) | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 500 °C | Thermal conductivity of 36.1 W/(m·K) | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 600 °C | Thermal conductivity of 33.8 W/(m·K) | normalized and stress-relieved | EN 10028-3 | Sheet | - |
Thermal diffusivity | -100 °C | Thermal diffusivity of 11.9 mm²/s | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 20 °C | Thermal diffusivity of 11 mm²/s | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 100 °C | Thermal diffusivity of 10.5 mm²/s | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 200 °C | Thermal diffusivity of 9.9 mm²/s | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 300 °C | Thermal diffusivity of 9.1 mm²/s | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 400 °C | Thermal diffusivity of 8.1 mm²/s | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 500 °C | Thermal diffusivity of 6.9 mm²/s | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 600 °C | Thermal diffusivity of 5.7 mm²/s | normalized and stress-relieved | EN 10028-3 | Sheet | - |
EN 10028-3 Grade P460N normalized and stress-relieved chemical
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | Aluminium of 0.005 % | normalized and stress-relieved | EN 10028-3 | Sheet |
Carbon | Carbon of 0.2 | normalized and stress-relieved | EN 10028-3 | Sheet |
Chromium | Chromium of 0.3 | normalized and stress-relieved | EN 10028-3 | Sheet |
Copper | Copper of 0.2 | normalized and stress-relieved | EN 10028-3 | Sheet |
Manganese | Manganese of 1 - 1.7 % | normalized and stress-relieved | EN 10028-3 | Sheet |
Molybdenum | Molybdenum of 0.1 | normalized and stress-relieved | EN 10028-3 | Sheet |
Nickel | Nickel of 0.4 | normalized and stress-relieved | EN 10028-3 | Sheet |
Nitrogen | Nitrogen of 0.025 | normalized and stress-relieved | EN 10028-3 | Sheet |
Phosphorus | Phosphorus of 0.03 | normalized and stress-relieved | EN 10028-3 | Sheet |
Silicon | Silicon of 0.1 - 0.6 % | normalized and stress-relieved | EN 10028-3 | Sheet |
Sulfur | Sulfur of 0.02 | normalized and stress-relieved | EN 10028-3 | Sheet |
Vanadium | Vanadium of 0.1 - 0.2 % | normalized and stress-relieved | EN 10028-3 | Sheet |
EN 10028-3 Grade P460N normalized and stress-relieved magnetic
Property | Value | Comment |
---|---|---|
Curie temperature | Curie temperature of 770 °C | Typical for Low Carbon Steel |
EN 10028-3 Grade P460N normalized and stress-relieved electrical
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Electrical resistivity | -100 °C | Electrical resistivity of 1.97e-07 Ω·m | normalized and stress-relieved | EN 10028-3 | Sheet |
- | 20 °C | Electrical resistivity of 2.62e-07 Ω·m | normalized and stress-relieved | EN 10028-3 | Sheet |
- | 100 °C | Electrical resistivity of 3.13e-07 Ω·m | normalized and stress-relieved | EN 10028-3 | Sheet |
- | 200 °C | Electrical resistivity of 3.85e-07 Ω·m | normalized and stress-relieved | EN 10028-3 | Sheet |
- | 300 °C | Electrical resistivity of 4.7e-07 Ω·m | normalized and stress-relieved | EN 10028-3 | Sheet |
- | 400 °C | Electrical resistivity of 5.69e-07 Ω·m | normalized and stress-relieved | EN 10028-3 | Sheet |
- | 500 °C | Electrical resistivity of 6.85e-07 Ω·m | normalized and stress-relieved | EN 10028-3 | Sheet |
- | 600 °C | Electrical resistivity of 8.2e-07 Ω·m | normalized and stress-relieved | EN 10028-3 | Sheet |
EN 10028-3 Grade P460N normalized and stress-relieved mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastic modulus | -100 °C | Elastic modulus of 217 GPa | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 20 °C | Elastic modulus of 200 - 212 GPa | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 20 °C | Elastic modulus of 200 GPa | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 20 °C | Elastic modulus of 212 GPa | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 100 °C | Elastic modulus of 207 GPa | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 200 °C | Elastic modulus of 199 GPa | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 300 °C | Elastic modulus of 192 GPa | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 400 °C | Elastic modulus of 184 GPa | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 500 °C | Elastic modulus of 175 GPa | normalized and stress-relieved | EN 10028-3 | Sheet | - |
- | 600 °C | Elastic modulus of 164 GPa | normalized and stress-relieved | EN 10028-3 | Sheet | - |
Poisson's ratio | 20 °C | Poisson's ratio of 0.29 [-] | normalized and stress-relieved | EN 10028-3 | Sheet | - |
Shear modulus | - | Shear modulus of 82 GPa | - | - | - | Typical for Low Carbon Steel |
Our rigorous quality control measures guarantee the reliability and consistency of our steel products.
-- Our promise
Similar or equivalent steel materials
- EN 10025-2 Grade S355J2 normalized or normalized formed (+N)
- EN 10028-3 Grade P460NL1 normalized or normalized formed (+N)
- EN 10028-3 Grade P460NL2 normalized or normalized formed (+N)
- EN 10028-3 Grade P460NH normalized or normalized formed (+N)
- ASTM A612 As-Rolled or Normalized and/or Stress Relieved
- EN 10217-3 Grade StE 460 normalized or normalized formed (+N)
- DIN 17125 Grade StE460 normalized or normalized formed (+N)
- EN 10216-3 Grade P460N normalized or normalized formed (+N)
- DIN 5512-1 Grade S355J2G3 normalized or normalized formed (+N)
- EN 10217-3 Grade P460N normalized or normalized formed (+N)
Get a quote