EN 10209 Grade DC03ED cold rolled, skin passed
EN 10209 Grade DC03ED cold rolled, skin passed introduction
Cold rolled low carbon steel for flat products for vitreous enamelling (direct enamelling, as well as for special applications of conventional two coat enamelling for better sag resistance).
Application: domestic appliances (cooking, laundry), sanitary ware (bathtubs, shower trays, sinks), architectural panels (interior and exterior), signage,The soft unalloyed steel DCO1ED, mat. No. 1.0399, is a cold formable steel and suitable for direct enameling as well as for special conventional applications of two-coat enameling, especially if there should be preferably enameled non deforming. In this case are necessary special measures in order to improve enamel`s adhesion. Mechanical specific values and freedom of stretcher strains are warranted for 6 months.
Application: simple reforming parts
pots, pans, covering caps for gas kitchen stoves, baking sheets, simple shower bases etc.
Welding: DC01ED is weldable acc. to the fusion welding methods:
MAG (metal active gas/plasma welding
arc hand welding
laser welding
gas welding
resistance welding (spot, roll seam, buckle welding)
Equivalent material: DIN ED3, JIS SPP, ASTM I, DIN 1.0399, DIN FeD 3, DIN CR1, DIN CR3, DIN DC03ED, AFNOR DC03ED, BS DC03ED, BS CR1, BS CR3, EN 1.0399
EN 10209 Grade DC03ED cold rolled, skin passed general
Property |
Temperature |
Value |
Comment |
Density |
20.0 °C |
Density of 7.8 - 7.9 g/cm³ |
Typical for Low Carbon Steel |
EN 10209 Grade DC03ED cold rolled, skin passed thermal
Property |
Temperature |
Value |
Comment |
Coefficient of thermal expansion |
20.0 °C |
Coefficient of thermal expansion of 1.32E-5 - 1.38E-5 1/K |
Typical for Low Carbon Steel |
Melting point |
- |
Melting point of 1480 - 1526 °C |
Typical for Low Carbon Steel |
EN 10209 Grade DC03ED cold rolled, skin passed chemical
Property |
Value |
Carbon |
Carbon of 4E-3 % |
Manganese |
Manganese of 0.4 % |
Phosphorus |
Phosphorus of 0.04 % |
Sulfur |
Sulfur of 0.05 % |
EN 10209 Grade DC03ED cold rolled, skin passed electrical
Property |
Value |
Comment |
Curie temperature |
Curie temperature of 770 °C |
Typical for Low Carbon Steel |
EN 10209 Grade DC03ED cold rolled, skin passed mechanical
Property |
Temperature |
Value |
Comment |
Elastic modulus |
20.0 °C |
Elastic modulus of 200 - 215 GPa |
Typical for Low Carbon Steel |
Elongation A80 |
20.0 °C |
Elongation A80 of 34 % |
- |
Elongation A80, transverse |
20.0 °C |
Elongation A80, transverse of 30 - 34 % |
- |
Poisson's ratio |
20.0 °C |
Poisson's ratio of 0.29 [-] |
Typical for Low Carbon Steel |
Tensile strength |
20.0 °C |
Tensile strength of 270 - 370 MPa |
- |
Tensile strength, transverse |
20.0 °C |
Tensile strength, transverse of 270 - 370 MPa |
- |
Yield strength |
20.0 °C |
Yield strength of 140 - 240 MPa |
- |
Yield strength, transverse |
20.0 °C |
Yield strength, transverse of 140 - 280 MPa |
- |