JIS G4303 Grade SUS316J1L solution treated
Equivalent material: DIN 1.4435, DIN X2CrNiMo18-14-3, AFNOR Z3CND17-12-03, AFNOR Z3CND18-14-03, BS 316S11, BS 316S13, BS 316S31, UNI X2CrNiMo1712, SS 2353, UNE X2CrNiMo18-14-3, AISI 316L, AISI 316LMo, SAE 316L, SAE 316LMo, JIS SUS316L, JIS SUS316LTBS, JIS SUS316LTP, JIS SUS316LTPY, JIS SUS316LTB, JIS SUSY316L, JIS SUSY316J1L, EN X2CrNiMo18-14-3, EN 1.4435, GOST 03Ch17N14M3, GB 00Cr18Ni15Mo3, UNS S31603
JIS G4303 Grade SUS316J1L solution treated general
Property |
Temperature |
Value |
Comment |
Density |
23.0 °C |
Density of 7.9 - 8.2 g/cm³ |
Typical for Austenitic Stainless Steel |
JIS G4303 Grade SUS316J1L solution treated thermal
Property |
Temperature |
Value |
Comment |
Coefficient of thermal expansion |
23.0 °C |
Coefficient of thermal expansion of 1.7E-5 - 1.9E-5 1/K |
Typical for Austenitic Stainless Steel |
Melting point |
- |
Melting point of 1230 - 1480 °C |
Typical for Austenitic Stainless Steel |
Specific heat capacity |
23.0 °C |
Specific heat capacity of 440 J/(kg·K) |
Typical for Austenitic Stainless Steel |
Thermal conductivity |
23.0 °C |
Thermal conductivity of 11 - 21 W/(m·K) |
Typical for Austenitic Stainless Steel |
JIS G4303 Grade SUS316J1L solution treated electrical
Property |
Temperature |
Value |
Comment |
Electrical resistivity |
23.0 °C |
Electrical resistivity of 8.5E-7 Ω·m |
Typical for Austenitic Stainless Steel |
JIS G4303 Grade SUS316J1L solution treated mechanical
Property |
Temperature |
Value |
Comment |
Elastic modulus |
23.0 °C |
Elastic modulus of 195 GPa |
Typical for Austenitic Stainless Steel |
Elongation A5 |
23.0 °C |
Elongation A5 of 40 % |
- |
Hardness, Brinell |
23.0 °C |
Hardness, Brinell of 187 [-] |
- |
Hardness, Rockwell B |
23.0 °C |
Hardness, Rockwell B of 90 [-] |
- |
Hardness, Vickers |
23.0 °C |
Hardness, Vickers of 200 [-] |
- |
Poisson's ratio |
23.0 °C |
Poisson's ratio of 0.3 [-] |
Typical for Austenitic Stainless Steel |
Reduction of area |
23.0 °C |
Reduction of area of 60 % |
- |
Shear modulus |
23.0 °C |
Shear modulus of 77 GPa |
Typical for Austenitic Stainless Steel |
Tensile strength |
23.0 °C |
Tensile strength of 480 MPa |
- |
Yield strength Rp0.2 |
23.0 °C |
Yield strength Rp0.2 of 175 MPa |
- |
Experience the strength, resilience, and versatility of our premium steel products.