ISO 4957 Grade X40CrMoV5-1 soft annealed (+A)

ISO 4957 Grade X40CrMoV5-1 soft annealed (+A) introduction

High-Cr-Mo-V-alloyed hot working steel with best tempering resistance and hot wear resistance as well as excellent heat resistance at moderate cooling and resistant to high temperature erosion by liquid metals.
Application:
high stressed mouldings for light metals, extruding tools of many kind, high wear loaded dies, shears for hot cutting

Equivalent material: GB 4Cr5MoSiV, CSN 19554, AFNOR Z40CDV5, BS BH13, GOST 4Ch5MF1S, ISO 40CrMoV5, UNI X40CrMoV5-11KU, JIS SKD61, PN WCLV, STAS 40VSiMoCr52, SS 2242, UNE F.5318, MSZ K13, SAE H13, DIN 1.2344, AFNOR X40CrMoV5-1, BS X40CrMoV5-1, UNI X40CrMoV511KU, UNE X40CrMoV5, AISI H13, EN X40CrMoV5-1, EN X40CrMoV511, EN 1.2344, ISO X40CrMoV5-1, GB 4Cr5MoSiV1, GB/T SM4Cr5MoSiV1, GB/T T22052, GB/T 4Cr5MoSiV1, GB/T T20502, GB/T 4c5MoSiV1, ASTM Type H13, UNS T20813

ISO 4957 Grade X40CrMoV5-1 soft annealed (+A) general

Property Temperature Value
Density 20.0 °C Density of 7.74 g/cm³

ISO 4957 Grade X40CrMoV5-1 soft annealed (+A) thermal

Property Temperature Value Comment
Coefficient of thermal expansion -100.0 °C Coefficient of thermal expansion of 1E-5 1/K -
- 20.0 °C Coefficient of thermal expansion of 1.08E-5 1/K -
- 100.0 °C Coefficient of thermal expansion of 1.13E-5 1/K -
- 200.0 °C Coefficient of thermal expansion of 1.18E-5 1/K -
- 300.0 °C Coefficient of thermal expansion of 1.23E-5 1/K -
- 400.0 °C Coefficient of thermal expansion of 1.27E-5 1/K -
- 500.0 °C Coefficient of thermal expansion of 1.3E-5 1/K -
- 600.0 °C Coefficient of thermal expansion of 1.32E-5 1/K -
Melting point - Melting point of 1370 - 1425 °C Typical for Tool And Machining Steel
Specific heat capacity 20.0 °C Specific heat capacity of 461 J/(kg·K) -
- 100.0 °C Specific heat capacity of 479 J/(kg·K) -
- 200.0 °C Specific heat capacity of 499 J/(kg·K) -
- 300.0 °C Specific heat capacity of 517 J/(kg·K) -
- 400.0 °C Specific heat capacity of 536 J/(kg·K) -
- 500.0 °C Specific heat capacity of 558 J/(kg·K) -
- 600.0 °C Specific heat capacity of 587 J/(kg·K) -
Thermal conductivity 20.0 °C Thermal conductivity of 19.2 W/(m·K) -
- 100.0 °C Thermal conductivity of 20.1 W/(m·K) -
- 200.0 °C Thermal conductivity of 22.4 W/(m·K) -
- 300.0 °C Thermal conductivity of 24 W/(m·K) -
- 400.0 °C Thermal conductivity of 25.1 W/(m·K) -
- 500.0 °C Thermal conductivity of 25.8 W/(m·K) -
- 600.0 °C Thermal conductivity of 26.1 W/(m·K) -
Thermal diffusivity 20.0 °C Thermal diffusivity of 5.4 mm²/s -
- 100.0 °C Thermal diffusivity of 5.3 mm²/s -
- 200.0 °C Thermal diffusivity of 5.5 mm²/s -
- 300.0 °C Thermal diffusivity of 5.5 mm²/s -
- 400.0 °C Thermal diffusivity of 5.4 mm²/s -
- 500.0 °C Thermal diffusivity of 5 mm²/s -
- 600.0 °C Thermal diffusivity of 4.4 mm²/s -

ISO 4957 Grade X40CrMoV5-1 soft annealed (+A) chemical

Property Value
Carbon Carbon of 0.37 - 0.43 %
Chromium Chromium of 4.8 - 5.5 %
Manganese Manganese of 0.3 - 0.5 %
Molybdenum Molybdenum of 1.2 - 1.5 %
Phosphorus Phosphorus of 0.03 %
Silicon Silicon of 0.9 - 1.2 %
Sulfur Sulfur of 0.03 %
Vanadium Vanadium of 0.9 - 1.1 %

ISO 4957 Grade X40CrMoV5-1 soft annealed (+A) electrical

Property Temperature Value
Electrical resistivity 20.0 °C Electrical resistivity of 5.43E-7 Ω·m
- 100.0 °C Electrical resistivity of 6.38E-7 Ω·m
- 200.0 °C Electrical resistivity of 7.05E-7 Ω·m
- 300.0 °C Electrical resistivity of 7.82E-7 Ω·m
- 400.0 °C Electrical resistivity of 8.68E-7 Ω·m
- 500.0 °C Electrical resistivity of 9.6E-7 Ω·m
- 600.0 °C Electrical resistivity of 1.06E-6 Ω·m

ISO 4957 Grade X40CrMoV5-1 soft annealed (+A) mechanical

Property Temperature Value Comment
Elastic modulus 20.0 °C Elastic modulus of 210 GPa -
Poisson's ratio 20.0 °C Poisson's ratio of 0.28 [-] -
Shear modulus 23.0 °C Shear modulus of 79 GPa Typical for Tool And Machining Steel