ISO 4957 Grade X32CrMoV3-3 soft annealed (+A)

ISO 4957 Grade X32CrMoV3-3 soft annealed (+A) introduction

Very tempering resistant Cr-Mo-V-alloyed universal applicable hot working steel with excellent low sensitivity to alternate temperatures, good sinkability and good water coolable.
Application:
liquid cooled forging and pressing tools for the steel and non ferrous metal forming, diecasting tools for brass and light metal processing die tools

Equivalent material: CSN 19541, AFNOR 32CDV12-28, BS BH10, GOST 3Ch3M3F, ISO 30CrMoV3, UNI 30CrMoV12-27KU, JIS SKD7, PN WLV, STAS 31VMoCr29, UNE F.5313, MSZ K14, SAE H10, DIN X32CrMoV12-28, DIN 1.2365, DIN 32CrMoV12-28, BS 32CrMoV12-28, AISI H10, EN 32CrMoV12-28, EN 32CDV12-28, EN 1.2365, ISO 32CrMoV12-28, GB/T 4Cr3Mo3SiV, GB/T T20303, ASTM Type H10, UNS T20810

ISO 4957 Grade X32CrMoV3-3 soft annealed (+A) general

Property Temperature Value
Density 20.0 °C Density of 7.74 g/cm³

ISO 4957 Grade X32CrMoV3-3 soft annealed (+A) thermal

Property Temperature Value Comment
Coefficient of thermal expansion -100.0 °C Coefficient of thermal expansion of 1E-5 1/K -
- 20.0 °C Coefficient of thermal expansion of 1.08E-5 1/K -
- 100.0 °C Coefficient of thermal expansion of 1.13E-5 1/K -
- 200.0 °C Coefficient of thermal expansion of 1.18E-5 1/K -
- 300.0 °C Coefficient of thermal expansion of 1.23E-5 1/K -
- 400.0 °C Coefficient of thermal expansion of 1.27E-5 1/K -
- 500.0 °C Coefficient of thermal expansion of 1.3E-5 1/K -
- 600.0 °C Coefficient of thermal expansion of 1.32E-5 1/K -
Max service temperature, long - Max service temperature, long of 0 - 600 °C -
Melting point - Melting point of 1370 - 1425 °C Typical for Tool And Machining Steel
Specific heat capacity 20.0 °C Specific heat capacity of 461 J/(kg·K) -
- 100.0 °C Specific heat capacity of 479 J/(kg·K) -
- 200.0 °C Specific heat capacity of 499 J/(kg·K) -
- 300.0 °C Specific heat capacity of 517 J/(kg·K) -
- 400.0 °C Specific heat capacity of 536 J/(kg·K) -
- 500.0 °C Specific heat capacity of 558 J/(kg·K) -
- 600.0 °C Specific heat capacity of 587 J/(kg·K) -
Thermal conductivity 20.0 °C Thermal conductivity of 19.2 W/(m·K) -
- 100.0 °C Thermal conductivity of 20.1 W/(m·K) -
- 200.0 °C Thermal conductivity of 22.4 W/(m·K) -
- 300.0 °C Thermal conductivity of 24 W/(m·K) -
- 400.0 °C Thermal conductivity of 25.1 W/(m·K) -
- 500.0 °C Thermal conductivity of 25.8 W/(m·K) -
- 600.0 °C Thermal conductivity of 26.1 W/(m·K) -
Thermal diffusivity 20.0 °C Thermal diffusivity of 5.4 mm²/s -
- 100.0 °C Thermal diffusivity of 5.3 mm²/s -
- 200.0 °C Thermal diffusivity of 5.5 mm²/s -
- 300.0 °C Thermal diffusivity of 5.5 mm²/s -
- 400.0 °C Thermal diffusivity of 5.4 mm²/s -
- 500.0 °C Thermal diffusivity of 5 mm²/s -
- 600.0 °C Thermal diffusivity of 4.4 mm²/s -

ISO 4957 Grade X32CrMoV3-3 soft annealed (+A) chemical

Property Value
Carbon Carbon of 0.28 - 0.35 %
Chromium Chromium of 2.7 - 3.2 %
Manganese Manganese of 0.15 - 0.45 %
Molybdenum Molybdenum of 2.6 - 3 %
Phosphorus Phosphorus of 0.03 %
Silicon Silicon of 0.1 - 0.4 %
Sulfur Sulfur of 0.03 %
Vanadium Vanadium of 0.4 - 0.7 %

ISO 4957 Grade X32CrMoV3-3 soft annealed (+A) electrical

Property Temperature Value
Electrical resistivity 20.0 °C Electrical resistivity of 5.43E-7 Ω·m
- 100.0 °C Electrical resistivity of 6.38E-7 Ω·m
- 200.0 °C Electrical resistivity of 7.05E-7 Ω·m
- 300.0 °C Electrical resistivity of 7.82E-7 Ω·m
- 400.0 °C Electrical resistivity of 8.68E-7 Ω·m
- 500.0 °C Electrical resistivity of 9.6E-7 Ω·m
- 600.0 °C Electrical resistivity of 1.06E-6 Ω·m

ISO 4957 Grade X32CrMoV3-3 soft annealed (+A) mechanical

Property Temperature Value Comment
Elastic modulus 20.0 °C Elastic modulus of 210 GPa -
Poisson's ratio 20.0 °C Poisson's ratio of 0.28 [-] -
Shear modulus 23.0 °C Shear modulus of 79 GPa Typical for Tool And Machining Steel