ISO 4957 Grade S18-1-2-5 quenched (+Q)
ISO 4957 Grade S18-1-2-5 quenched (+Q) introduction
Tough high alloyed W-Co high speed steel with high hot hardness.
Application: turning, planing and blow tools, scrub cutter
Equivalent material: GB W18Cr4VCo5, CSN 19855, AFNOR Z80WKCV18-05-04-01, BS BT4, GOST R18K5F2, ISO HS18-1-1-5, UNI HS18-1-1-5, JIS SKH3, STAS Rp2, UNE F.5530, DIN 1.3255, AISI T4, SAE T4, EN 1.3255, ASTM Type T4, UNS T12004
ISO 4957 Grade S18-1-2-5 quenched (+Q) general
Property |
Temperature |
Value |
Density |
20.0 °C |
Density of 8.12 g/cm³ |
ISO 4957 Grade S18-1-2-5 quenched (+Q) thermal
Property |
Temperature |
Value |
Comment |
Coefficient of thermal expansion |
-100.0 °C |
Coefficient of thermal expansion of 9.6E-6 1/K |
- |
- |
20.0 °C |
Coefficient of thermal expansion of 1.05E-5 1/K |
- |
- |
100.0 °C |
Coefficient of thermal expansion of 1.11E-5 1/K |
- |
- |
200.0 °C |
Coefficient of thermal expansion of 1.16E-5 1/K |
- |
- |
300.0 °C |
Coefficient of thermal expansion of 1.2E-5 1/K |
- |
- |
400.0 °C |
Coefficient of thermal expansion of 1.24E-5 1/K |
- |
- |
500.0 °C |
Coefficient of thermal expansion of 1.27E-5 1/K |
- |
- |
600.0 °C |
Coefficient of thermal expansion of 1.3E-5 1/K |
- |
Melting point |
- |
Melting point of 1370 - 1425 °C |
Typical for Tool And Machining Steel |
Specific heat capacity |
23.0 °C |
Specific heat capacity of 420 - 460 J/(kg·K) |
Typical for Tool And Machining Steel |
Thermal conductivity |
20.0 °C |
Thermal conductivity of 27.6 W/(m·K) |
- |
- |
100.0 °C |
Thermal conductivity of 27.9 W/(m·K) |
- |
- |
200.0 °C |
Thermal conductivity of 27.7 W/(m·K) |
- |
- |
300.0 °C |
Thermal conductivity of 27.5 W/(m·K) |
- |
- |
400.0 °C |
Thermal conductivity of 27 W/(m·K) |
- |
- |
500.0 °C |
Thermal conductivity of 26.6 W/(m·K) |
- |
- |
600.0 °C |
Thermal conductivity of 26.1 W/(m·K) |
- |
ISO 4957 Grade S18-1-2-5 quenched (+Q) chemical
Property |
Value |
Carbon |
Carbon of 0.75 - 0.83 % |
Chromium |
Chromium of 3.8 - 4.5 % |
Cobalt |
Cobalt of 4.5 - 5 % |
Manganese |
Manganese of 0.4 % |
Molybdenum |
Molybdenum of 0.5 - 0.8 % |
Phosphorus |
Phosphorus of 0.03 % |
Silicon |
Silicon of 0.45 % |
Sulfur |
Sulfur of 0.03 % |
Tungsten |
Tungsten of 17.5 - 18.5 % |
Vanadium |
Vanadium of 1.4 - 1.7 % |
ISO 4957 Grade S18-1-2-5 quenched (+Q) electrical
Property |
Temperature |
Value |
Electrical resistivity |
20.0 °C |
Electrical resistivity of 5.24E-7 Ω·m |
- |
100.0 °C |
Electrical resistivity of 5.81E-7 Ω·m |
- |
200.0 °C |
Electrical resistivity of 6.64E-7 Ω·m |
- |
300.0 °C |
Electrical resistivity of 7.51E-7 Ω·m |
- |
400.0 °C |
Electrical resistivity of 8.44E-7 Ω·m |
- |
500.0 °C |
Electrical resistivity of 9.41E-7 Ω·m |
- |
600.0 °C |
Electrical resistivity of 1.04E-6 Ω·m |
ISO 4957 Grade S18-1-2-5 quenched (+Q) mechanical
Property |
Temperature |
Value |
Comment |
Elastic modulus |
20.0 °C |
Elastic modulus of 224 GPa |
- |
- |
100.0 °C |
Elastic modulus of 220 GPa |
- |
- |
200.0 °C |
Elastic modulus of 214 GPa |
- |
- |
300.0 °C |
Elastic modulus of 207 GPa |
- |
- |
400.0 °C |
Elastic modulus of 199 GPa |
- |
- |
500.0 °C |
Elastic modulus of 191 GPa |
- |
- |
600.0 °C |
Elastic modulus of 180 GPa |
- |
Poisson's ratio |
20.0 °C |
Poisson's ratio of 0.28 [-] |
- |
Shear modulus |
23.0 °C |
Shear modulus of 79 GPa |
Typical for Tool And Machining Steel |