EN 10083-1 Grade 42CrMoS4 surface hardened

Equivalent material: ISO 42CrMoS4, ASTM A29 Grade 4140, ASTM A304 Grade 4140H, ASTM A434 Grade 4140, SAE 4140H, UNS H41400, EN 1.7227, DIN 1.7227, DIN 42CrMoS4, AISI 4140, SAE 4140, ASTM Grade B7, ASTM Grade 12, ASTM Grade 7M, UNS G41400

EN 10083-1 Grade 42CrMoS4 surface hardened general

Property Temperature Value
Density 20.0 °C Density of 7.85 g/cm³

EN 10083-1 Grade 42CrMoS4 surface hardened thermal

Property Temperature Value Comment
Coefficient of thermal expansion 100.0 °C Coefficient of thermal expansion of 1.11E-5 1/K -
- 200.0 °C Coefficient of thermal expansion of 1.21E-5 1/K -
- 300.0 °C Coefficient of thermal expansion of 1.29E-5 1/K -
- 400.0 °C Coefficient of thermal expansion of 1.35E-5 1/K -
Melting point - Melting point of 1382 - 1529 °C Typical for Chromium Molybdenum Steel
Specific heat capacity 20.0 °C Specific heat capacity of 460 J/(kg·K) -
Thermal conductivity 20.0 °C Thermal conductivity of 42 W/(m·K) -

EN 10083-1 Grade 42CrMoS4 surface hardened chemical

Property Value
Carbon Carbon of 0.38 - 0.45 %
Chromium Chromium of 0.9 - 1.2 %
Copper Copper of 0.4 %
Manganese Manganese of 0.6 - 0.9 %
Molybdenum Molybdenum of 0.15 - 0.3 %
Phosphorus Phosphorus of 0.03 %
Silicon Silicon of 0.1 - 0.4 %
Sulfur Sulfur of 0.02 - 0.04 %

EN 10083-1 Grade 42CrMoS4 surface hardened electrical

Property Temperature Value
Electrical resistivity 20.0 °C Electrical resistivity of 1.9E-7 Ω·m

EN 10083-1 Grade 42CrMoS4 surface hardened mechanical

Property Temperature Value
Elastic modulus 20.0 °C Elastic modulus of 210 GPa
- 100.0 °C Elastic modulus of 205 GPa
- 200.0 °C Elastic modulus of 195 GPa
- 300.0 °C Elastic modulus of 185 GPa
Poisson's ratio 20.0 °C Poisson's ratio of 0.28 [-]
Shear modulus 20.0 °C Shear modulus of 81 GPa